Condizioni deumidificazione polimeri
Polimero | Densità apparente gr/cm3 |
Tempo Ore | Temperatura °C |
ABS | 0.6 | 2 | 80 |
CA | 0.75 | 2 | 70 |
CAB | 0.65 | 2 | 70 |
EVA | 0.57 | 2 | 90 |
EVOH | 0.70 | 2 | 90 |
IM | 0.56 | 3 | 60 |
LCP | 0.75 | 3 | 150 |
PA11 – PA12 | 0.6 | 3 | 70 |
PA6 – PA66 – PA46 | 3 | 90 | |
PAI | 0.85 | 6 | 180 |
PAR | 0.70 | 5 | 120 |
PBT | 0.78 | 3 | 130 |
PC | 0.75 | 2 | 120 |
PC/ABS | 3 | 100 | |
PC/PBT | 3 | 110 | |
PE | 0.55 | 1 | 85 |
PEEK | 0.75 | 3 | 150 |
PEI | 4 | 140 | |
PEN | 5 | 140 | |
PES | 3 | 150 | |
PET | 3 | 130 | |
PI | 2 | 120 | |
PMMA | 3 | 80 | |
POM | 0.85 | 2 | 90 |
PP | 1 | 90 | |
PP TALCO | 2 | 80 | |
PPO | 2 | 100 | |
PPS | 2 | 130 | |
PS | 1 | 80 | |
PSU | 3 | 120 | |
PTT | 4 | 130 | |
PUR | 2 | 70 | |
PVC | 1 | 70 | |
SAN | 2 | 80 | |
SB | 1 | 80 | |
TPV | 2 | 110 | |
TPC-ET | 2 | 80 | |
TPO-POE | 3 | 70 | |
TPU | 2 | 70 |